STUDY OF PHOTOLUMINESCENCE INHOMOGENEITY IN InGaN QUANTUM WELLS WITH CAPPING LAYERS OF DIFFERENT THICKNESS

Ieva Šimonytė1

1 Semiconductor Physics Department, Vilnius University, Saulėtekio 9-III, LT-10222 Vilnius, Lithuania

Group-III nitrides have attracted a considerable attention for their various use in optoelectronics. The ternary InGaN alloy is the primary compound in commercial production of blue and green light-emitting diodes (LEDs) and laser diodes. A white LED that is currently produced by combining a blue LED with yellow phosphor offers a replacement for conventional sources in general lighting. Though InGaN-based devices have been developed and used on a large scale, photoluminescence inhomogeneity in InGaN quantum wells is still not clearly understood.

Inhomogeneous indium distribution in active layers generates spatial band gap fluctuations. Carrier localization in indium rich areas is beneficial for higher emission intensity. However, InGaN with high indium content exhibits a low quantum efficiency. This is the reason why III-nitride compounds are still not used in production of long-wavelengths LEDs [1].

In this work, spatial inhomogeneity of photoluminescence in InGaN quantum wells with different capping layers were studied. Six samples under study were grown by a MOCVD method and contained identical active layers consisting of five InGaN quantum wells. After growing the quantum wells, a 20 nm thick capping layer of n-type AlGaN was deposited on five samples. An additional capping layer of n-type GaN layers of 30, 60, 120, and 180 nm in thickness were deposited on four samples. Photoluminescence was studied with spatial and spectral resolution using confocal microscope coupled with a spectrometer. CW emission of He-Cd laser was used for excitation. In each sample, two randomly selected 30 x 30 μm2 areas have been scanned. Obtained PL intensity and peak wavelengths mappings were used in the further analysis of PL parameters.

Correlations between PL intensity, peak position, and full width at half maximum (FWHM) were calculated for each sample. Small correlation between peak intensity and FWHM was observed in the samples, where the averaged PL intensity is higher. The correlation is the stronger the higher is the averaged PL intensity. Correlation between PL intensity and FWHM is stronger. Strong anticorrelation was observed in the samples with the highest intensity. The anticorrelation becomes smaller in the samples, where the intensity is smaller. The anticorrelation shows that the PL band in bright areas have a larger band width.

The values of Spearman's and Pearson's correlation coefficients are small and do not reveal any statistically reliable correlation between the peak position and PL intensity in samples with 60, 120, and 180 nm thick GaN capping layers. Small correlation was observed in samples with 30 nm thick GaN layer, without the GaN layer, and with no capping layer at all. In samples where correlation was small, integrated PL spectra from bright areas was slightly (~3 nm) redshifted in respect of the integrated PL spectra from dark areas.

The analysis of the averaged spatially integrated PL intensity from each sample revealed that the integrated PL intensity is a nonmonotonous function of GaN capping layer thickness. The highest PL intensity was observed in the sample with the GaN capping layer of ~100 nm in thickness.


[1] K. Okamoto, A. Kaneta, Y. Kawakami, S. Fujita, J. Choi, M. Terazima, T. Mukai, Confocal microphotoluminescence of InGaN-based light-emitting diodes. Journal of Applied Physics 98, 064503 (2005)