Light-emitting diodes (LEDs) with the ZnO-based active region have attracted considerable attention due to the great structural and physical properties and relatively low production costs of ZnO, compared to GaN [1]. The band gap tunability from ultra-violet to yellow spectral range can be achieved. By alloying ZnO with Be or Mg the band gap is increasing, while by alloying it with Cd, the band gap is decreasing [2]. Band gap engineering is an important step for the development of multiple quantum wells (MQWs) structures, which improve LEDs performance by enhancing radiative recombination rate of excitons.
Optical properties of 6 LED samples were investigated in this experiment. In each sample, the Ga-doped ~30 nm thick n-ZnO cap layer and three periods of CdZnO/ZnO QWs (~5 nm thick CdZnO wells separated by ~20 nm thick ZnO barriers) were grown on a p-GaN (~1 μm), which was deposited on a u-GaN template of ~2 μm in thickness on c-plane sapphire substrate. The p-GaN and u-GaN layers were grown using metalorganic chemical vapour deposition (MOCVD), whereas MBE method was used for MQWs and the cap layer growth. Cd effusion cell and substrate temperatures were varied for different samples when growing well (barrier) layers. The samples were fabricated in the Institute of Photonics and Optoelectronics of National Taiwan University.
The temperature dependent photoluminescence (PL) spectra of the samples were measured using laser diode ($\lambda_{\text{exc}}$ = 403 nm) as an excitation source, suitable for selective excitation of CdZnO MQWs. The laser spot diameter was estimated to be around 200 μm on the surface of the sample. PL signal was dispersed using a monochromator (Jobin Yvon HRD-1) with holographic diffraction gratings, having 1200 grooves/mm, and registered using a photomultiplier tube (Hamamatsu R1463P). Cooling of the samples was performed using a closed-circuit He cryostat, which allows temperature of the sample to be changed in the interval from 8 K to 300 K. Samples' temperature was stabilized with the help of a proportional-integral-derivative controller. During the measurement temperature fluctuations did not exceed 1% deviation.
PL spectra of CdZnO/ZnO MQWs was further investigated by analyzing the temperature dependencies of PL peak position, PL intensity and full width at half maximum (FWHM). Varshni (1) and Bose-Einstein (2) equations were used to fit the PL peak position dependencies on temperature, considering the investigated PL peak being mostly influenced by near-band-edge emission from CdZnO MQWs.
$$E_{\text{g}}(T) = E_{\text{g}}(0) - \frac{\alpha T^2}{T + \beta}\tag{1}$$$$E_{\text{g}}(T) = E_{\text{g}}(0) - \frac{k}{\exp(\theta/T) - 1}\tag{2}$$Two models were used to fit PL intensity (I) temperature dependencies. Better fitting results with lower errors were obtained using the equation (3) with the hopping term added [3], if compared with the one without it (4).
$$I(T) = \frac{I_0}{1 + A\exp(-E_{\text{a}}/k_{\text{B}}T + T/T_{\text{B}})}\tag{3}$$$$I(T) = \frac{I_0}{1 + A\exp(-E_{\text{a}}/k_{\text{B}}T)}\tag{4}$$In case of FWHM ($\Gamma$) dependency on temperature, Hellman-O'Neill equation (5) was exploited. In this model, the greatest contribution to the behavior of FWHM on temperature is made by carrier interaction with phonons (both acoustic and optical).
$$\Gamma(T) = \Gamma_0 + \gamma_{\text{ph}}T + \frac{\Gamma_{\text{LO}}}{\exp(\hbar \omega_{\text{LO}}/k_{\text{B}}T) - 1}\tag{5}$$Furthermore, values of internal quantum efficiency (IQE) at 300 K were calculated, after the condition that IQE at 8 K is equal to 100 %. IQE defined in this way can represent the optical quality of MQWs. Evaluated IQE values varied from 11 % to 36 % for different samples.