Qualitative analysis of quantum structures designed for applications in light emitting diode (LED) fabrication is crucial for the development of more efficient samples through finding the best combination of technological steps involved in their epitaxial growth process. Photoluminescence (PL) measurements helps to qualify properties of light emitted from particular sample. Direct band gap semiconductive materials like ZnO and GaN along with their ternary alloys with Cd and In respectively, are widely investigated these days partly because of lack of efficient and high-brightness green LEDs that could be used in full-color displays or even in solid state lighting as a substitute for phosphor-based white LEDs.
Temperature-dependent PL results of 4 samples were investigated in this work. CdZnO/ZnO LEDs (2 samples) had active regions with 3 and 10 periods of CdZnO well layers separated with ZnO barriers. n-ZnO capping layer and the active region were grown using molecular beam epitaxy (MBE), whereas metalorganic chemical vapor deposition (MOCVD) was used for growing p-GaN buffer and u-GaN template layers. Active regions of other 2 samples consisted of 5 periods of InGaN/GaN multiple quantum wells (MQWs) sandwitched between p-AlGaN (top) and n-GaN (bottom) buffer layers atop u-GaN template. Both buffer/template layers and active regions of these samples were grown using MOCVD. One of them also had an MBE-grown p-GaN capping layer. All mentioned samples were fabricated on a c-plane sapphire substrate in the Institute of Photonics and Optoelectronics of National Taiwan University.
Photoexcitation of the sample was performed using selective and non-selective excitation sources. Under selective excitation conditions, violet laser diode (LD) with $\lambda_{exc}=403$ nm was employed, whereas continues wave He-Cd laser ($\lambda_{exc}=325$ nm) was used for non-selective excitation. The laser spot diameter was estimated to be around 250 μm on the surface of the sample. PL signal was dispersed using a monochromator (Jobin Yvon HRD-1) with holographic diffraction gratings, having 1200 grooves/mm, and registered using a photomultiplier tube (Hamamatsu R1463P). Cooling of the samples was performed utilizing a closed-circuit He cryostat, which allows the temperature of the sample to be changed in the interval from 8 K to 300 K. Samples' temperature was stabilized with the help of a proportional-integral-derivative controller.
Effects like carrier localization, thermal quenching, line broadening and differences between selective and non-selective excitation were analized by carrying out the temperature dependencies of spectral peak position, intensity and linewidth of the peak originating from quantum well regions of samples. If compared with CdZnO/ZnO samples, InGaN/GaN MQWs exhibited more pronounced blueshift of spectral peak position on temperature. While this type of dependency can be considered as a fingerprint of carrier localization in quantum wells, it is convenient to use the density-of-states Gaussian band-tail model [1] to describe it qualitatively. Recombination mechanisms in InGaN/GaN MQWs can be attributed to the emission from localized band-tail states originating from quantum dot-like and phase-separated indium-rich regions in the wells. This carrier localization formed in the plane of the layers suppresses lateral carrier diffusion, thereby reducing the probability of carriers entering nonradiative recombination centers [2].
Internal quantum efficiencies (IQE) at room temperature were calculated from PL results after assumption that 8 K spectra reflects radiative recombination from MQWs. Values of IQE (300 K) varied from ~6% to ~14% for different samples and were a few percent larger for InGaN/GaN MQWs in comparrison with CdZnO/ZnO samples, which indicates poorer CdZnO wells structural quality.
Also, approximate values of Cd and In contents in CdxZn1-xO and InyGa1-yN alloys were calculated using relationship between band gap energies of constituent compounds and their molar fractions in ternary alloys (Vegard's law). For samples discussed in this work, Cd and In contents in MQWs were estimated to be around 15% and ~25% respectively. Mismatches between lattices of the constituents causes higher dislocation densities, which, in hand, intensifies the non-radiative recombination of excitons. Anyway, high Cd and In content is necessary in order to achieve green light emission from MQWs as ZnO and GaN are wide band gap semiconductors.