EVALUATION OF D AND G RAMAN MODES RATIO FOR THE ANALYSIS OF CARBON NANOTUBE STRUCTURE

Ieva Puodžiūtė1, Justinas Čeponkus1

1 Faculty of Physics, Vilnius University, Saulėtekio Ave. 9-III, LT-10222 Vilnius, Lithuania

Carbon nanotubes are very perspective and important materials in the field of physics, chemistry, medicine and material sciences. Scientists still face with a problem to analyse carbon characteristics from their spectra. The goal of this project is to study D and G modes intensity dependence on environment surrounding carbon nanotubes. We studied single-walled carbon nanotubes (SWCNT) and functionalized carbon nanotubes with carboxyl group (COOH) by the means of FT-Raman spectroscopy. FT-Raman with NIR excitation spectroscopy is easy, fast, cheap and precise method to study such complicated structures [1]. In FT-Raman spectrometers Nd:YAG laser (1064 nm) is usually used for the Raman excitation, the photon energy is too low to excite fluorescence. High sensitivity, high speed and possibility to average high number of spectral scans allow to observe even very weak spectral bands in the FT-Raman spectra.

The samples were prepared using “pallet” technique. Carbon materials were mixed with potassium-bromide (KBr) powder in different proportion and mechanical pressure of 10 ton per cm2 was applied. Measurements were performed using a FT-Raman spectrometer MultiRAM from “Bruker”. The spectra were measured in range of 3600 to 50 cm-1.

FT-Raman spectra of single-walled carbon nanotubes with different concentration of nanotubes in KBr pallet are presented in figure 1.

Figure 1
Fig. 1. FT-Raman spectra of SWCNT in Kbr: 1:1 – one part of SWCNT and one part of KBr; 2:1 – two parts of SWCNT and one part of KBr; 4:1 – four parts of SWCNT and one part of KBr.

The band at 1589 cm-1 (G mode) seems to be the most important one for characterization of carbon nanotubes. The band localized at 2551 cm-1 (G' mode) also is characteristic for carbon nanotubes and is attributed to the first overtone of 1589 cm-1 band. A low-frequency weak band at 171 cm-1 is attributed to the breathing mode (RBM – radial breathing mode) of nanotubes [1], but it is less suited for identification of carbon structures due to its weakness. The band at 1290 cm-1 (D mode), according to literature, describes the defects of carbon nanotubes [1, 2]. However during our measurements we noticed that this band intensity also depends on other factors.

Our results show that D modes intensity depends on proportion of nanotubes in KBr compound. As it can be seen in the figure 1, the intensity of D band in 2:1 concentration is different from this band intensity in 1:1 and 4:1 spectra. The dependence of D mode intensity from the nanotube to KBr ratio is not linear according to our observations. The intensity of this mode is also dependent from other factors such as moisture from the atmospheric water and possibly others environmental factors. Most likely explanation for such dependency could be that at some concentrations the interaction between the nanotubes itself and nanotubes and KBr powder is minimized due to the size ratios of KBr particles and nanotubes.


[1] T. Belin, F. Epron. Characterization methods of carbon nanotubes: a review, Materials Science and Engineering B, 119 (2005) 105-118.

[2] R.Schonfelder, et al. On the merits of Raman spectroscopy and thermogravimetric analysis to asses carbon nanotubes structural modifications, Applied Physics A, 106 (2012) 843-852.