Semiconductor compound GaBiAs is a promising material for ultrafast infrared light emitters and detectors for optical fiber systems and terahertz applications. Introducing a small content of bismuth into gallium arsenide significantly reduces the band gap of the compound. However, the growth of high quality GaBiAs is still a challenge. GaBiAs epitaxial layers with Bi content of up to 10% can be grown at low temperatures (~240-380°C).
In this work, the photoluminescence (PL) properties of GaBiAs epitaxial layers and GaBiAs/GaAs quantum wells were investigated with spatial resolution. To investigate the correlation of the surface morphology to the PL images, the same areas were additionally scanned by an atomic force microscope (AFM). The GaBiAs structures used in this study were grown by molecular beam epitaxy (MBE) technique on semi-insulating GaAs substrates at the Center for Physical Sciences and Technology, Vilnius, Lithuania. Six low-temperature grown samples were investigated: three epilayers and three multiple quantum well (MQW) structures with different Bi content. The approximate percentage of Bi in the epitaxial layers was determined according to the position of optical absorption edge while the Bi content in the MQW structures was found from the PL emission peak wavelength.
The PL spatial distribution of the samples was investigated using WITec Alpha 300S confocal microscope coupled to Andor spectrometer equipped with iDus InGaAs CCD. The spatial distributions of PL parameters were investigated by raster scanning randomly selected areas on the sample top surface. A red CW laser diode (emission wavelength at 660 nm) manufactured by Integrated Optics was used for excitation. The surface morphology of the samples was studied by an atomic force microscope (AFM) integrated in the WITec system. All the measurements were performed at room temperature.
The epitaxial layers exhibited PL bands peaked at 1088 nm, 1164 nm, and 1321 nm in the epilayers containing 5.4%, 6.3% and 7.0% of Bi, respectively. The highest PL intensity was recorded in the sample with the lowest Bi content. The PL spectrum of the epilayer with Bi content of 7.0% consists of two highly overlapping peaks at 1274 and 1321 nm, which is most probably related to microscale phase separation. The PL band undergoes a red shift and a decrease in intensity with increasing Bi content. All of the epilayers have a striped pattern of PL intensity spatial distribution. Such patterns are related to the corresponding structures in surface morphology, as it was observed by AFM. The patterns originate from thick layer relaxation. The epilayer with 6.3% of Bi showed a spotted pattern of PL intensity distribution in the smaller-scale images. This epilayer also exhibited the largest density of dislocation-related pits.
The MQW structures with approximate Bi content of 5.6%, 6.8% and 8.0% exhibited PL bands peaked at 1039 nm, 1112 nm, and 1191, respectively. The dependences of intensity and spectral position of the PL bands on Bi content are similar to those observed in the epilayers. However, the PL intensity degradation with increasing Bi fraction is not as abrupt for the MWQs. Most probably, the strained layers in the MQW structure are more resistant to the formation of point defects than the epitaxial layers are.
All of the MQW structures exhibited a modest density of dislocation related pits in the surface images. PL imaging revealed spots of lower emission intensity, which are associated with the dislocations. The MQW sample with the lowest Bi content exhibits a red shift of PL band at the pits. Therefore it is feasible that the dislocation threads are originating from the Bi-rich clusters inside quantum wells. On the contrary, for the rest of the MQW samples, a blue shift is observed at the dislocation pits. The shift in this case might be related to the decrease of quantum well width at the pits.
The MQW structure with the largest Bi content (8.0%) exhibits a smaller density of dislocation related pits than the sample with the moderate Bi percentage (6.8%), as opposed to the expectations. The reduction of dislocation density might be related to the decreased quantum well width and improved strain. Nevertheless, the PL intensity in this sample is lower, due to the influence of a larger density of point defects. Our results indicate that the increased density of point defects is in correlation with the defective notches on the surfaces of the MQW samples.