Recently, antimony selenoiodide (SbSeI), one of the chalcohalide semiconductors that belongs to V-VI-VII class materials has been the subject of growing interest for applications, such as, solar cells, X-ray and γ-ray detection, photocatalysis, and in other optoelectronic devices. SbSeI enjoys additional benefits compared to other PV thin film systems, including the earth abundant and low toxicity chemical composition, high thermodynamic stability and large absorption coefficient (up to 10\(^{5}\) cm\(^{-1}\)). Although SbSeI has very promising properties, there are few studies where this material has been used as an absorber layer in solar cells, and reported power conversion efficiency was low - 4,1 % [1]. One of the key challenges in synthesizing SbSeI thin film absorbers for PV application, is its tendency to form porous needle-like structure [2]. Because of quasi-1-dimensional crystalline structure of SbSeI, it has a preferred growth direction along [001] axis resulting in rod-shaped grain growth. The goal of this study is to find optimal annealing conditions to obtain continuous, uniform and compact morphology SbSeI thin films.
In this study we used a two-stage synthesis route where first precursor layers were deposited followed by annealing step. SbSeI precursors films were deposited under vacuum by thermal evaporation method to achieve amorphous, compact SbSeI thin film with Sb:Se:I molar ratio near 1:1:1. For crystallization stage, annealing under air atmosphere was performed with temperatures ranging from 140 \(^{o}\)C to 190 \(^{o}\)C with a graphite cover to prevent SbI\(_{3}\) vaporisation. Properties of SbSeI thin films were characterised by XRD (θ-θ, Bragg-Brentano geometry), SEM, EDX and photoluminescence spectroscopy.
In situ XRD results showed that crystallisation onset of SbSeI begins at 100 \(^{o}\)C , at the same time crystallinity of SbI\(_{3}\) phase increases. The turning point was found about 140-150 \(^{o}\)C, where steep drop in SbI\(_{3}\) and increase of SbSeI phases was observed. SEM images of top and cross-section showed that best compact morphology was achieved at lower in 160-165 \(^{o}\)C range. Photoluminescence studies revealed that PL signal was observed in samples annealed at temperature above 160 \(^{o}\)C and intensity increased with increasing annealing temperature.