SYNTHESIS AND CHARACTERIZATION OF NICKEL TUNGSTEN CATALYST

Lukas Šimkus1, Gitana Valeckytė1, Zita Sukackienė1, Jūratė Vaičiūnienė1, Loreta Tamašauskaitė-Tamašiūnaitė1, Eugenijus Norkus1

1 Center for Physical Sciences and Technology (FTMC), Department of Catalysis, Vilnius, Lithuania

Hydrogen is widely recognized as a key energy carrier for the transition toward a sustainable energy system [1,2]. However, the majority of hydrogen production currently relies on non-renewable fossil resources, resulting in significant carbon emissions [3]. While carbon capture technologies enable the transition from gray to blue hydrogen, truly sustainable green hydrogen production remains commercially limited [4]. As a result, alternative hydrogen generation routes that avoid direct CO\(_2\) emissions are of considerable interest. One promising approach is the hydrolysis of borohydrides, which enables efficient hydrogen release without carbon byproducts [5]. The effectiveness of this process strongly depends on the availability of cost-efficient and active catalysts, particularly those based on non-noble metals. In this context, electrolessly deposited nickel–tungsten catalysts supported on copper substrates represent a viable and scalable solution for borohydride-based hydrogen generation.

In the present study, the synthesis of Ni\(_{93}\)W\(_7\)/Cu, Ni\(_{91}\)W\(_9\)/Cu, Ni\(_{89}\)W\(_{11}\)/Cu, Ni\(_{87}\)W\(_{13}\)/Cu, and Ni\(_{85}\)W\(_{15}\)/Cu catalysts was accomplished through the chemical method of metal deposition. The surface morphology, internal structure and chemical composition of the obtained catalysts were analyzed using field emission scanning electron microscopy, X-ray photoelectron spectroscopy and inductively coupled plasma optical emission spectroscopy. It was determined that the prepared coating particles consist of oval-shaped agglomerates. The composition of the catalysts was analysed, showing Ni loading ranging from 252.0 to 603.5 µg/cm\(^2\) and W ranging from 43.0 to 64.9 µg/cm\(^2\).

The element al composition and metal loading of the prepared NiW/Cu coatings analyzed via ICP–OES.
CatalystElement, wt.%Element Loadings, \(\mu\)g cm\(^{-2}\)
2-6NiWNiWNi + W
Ni\(_{93}\)W\(_7\)/Cu92.947.09603.546.0649.5
Ni\(_{91}\)W\(_9\)/Cu91.138.87483.747.1530.8
Ni\(_{89}\)W\(_{11}\)/Cu89.0410.96527.064.9591.9
Ni\(_{87}\)W\(_{13}\)/Cu86.8813.12373.956.5430.4
Ni\(_{85}\)W\(_{15}\)/Cu85.4014.60252.043.0295.0

[1] P.-A. Le, V. D. Trung, P. L. Nguyen, T. V. B. Phung, J. Natsuki, and T. Natsuki, “The current status of hydrogen energy: an overview,” RSC Advances, vol. 13, no. 40, pp. 28262–28287, Jan. 2023, doi: 10.1039/d3ra05158g.

[2] D. Guan et al., “Hydrogen society: from present to future,” Energy & Environmental Science, vol. 16, no. 11, pp. 4926–4943, Jan. 2023, doi: 10.1039/d3ee02695g.

[3] M. Hermesmann and T. E. Müller, “Green, Turquoise, Blue, or Grey? Environmentally friendly Hydrogen Production in Transforming Energy Systems,” Progress in Energy and Combustion Science, vol. 90, p. 100996, Feb. 2022, doi: 10.1016/j.pecs.2022.100996.

[4] V. A. Panchenko, Yu. V. Daus, A. A. Kovalev, I. V. Yudaev, and Yu. V. Litti, “Prospects for the production of green hydrogen: Review of countries with high potential,” International Journal of Hydrogen Energy, vol. 48, no. 12, pp. 4551–4571, Oct. 2022, doi: 10.1016/j.ijhydene.2022.10.084.

[5] N. Ruslan et al., “Review on Magnesium hydride and sodium borohydride hydrolysis for hydrogen production,” Crystals, vol. 12, no. 10, p. 1376, Sep. 2022, doi: 10.3390/cryst12101376.