Biodegradable polymers represent a solution to the problems of contamination caused by conventional synthetic polymers. For this reason, starch is considered be one of the most promising substances due to its biodegradability, low cost and abundant availability. The starch application areas remain limited due to its poor resistance to water and no plastic behaviour under heating. Chemical modification of starch is one of the most attractive methods to reduce the number of hydrogen bonds and increase the hydrophobicity of starch.
The aim of this study was to synthesize thermoplastic starch esters with controllable properties by using organic anhydrides of different chemical composition and varying the degree of substitution (DS). Potato starch was modified with acetic (Ac) or/and octenyl succinic (OSA) anhydrides and characterized by Fourier-transform infrared spectroscopy and scanning electron microscopy. The hydrophobicity of starch acetate octenyl succinate was assessed by measuring water contact angle. The thermal properties of the modified starches were evaluated using thermogravimetry and differential scanning calorimetry.
For OSA starch with DSOSA=0.06 and starch acetate at low degree of substitution, DSAc being up to 0.62, the glass transition (Tg) temperature was not observed and the destruction temperature (Td) was decreasing with increasing of DSAc (Table 1). Starch acetate with high DSAc≥0.8 had Tg which is in the interval of 162-167 °C and Td was increasing with increasing DSAc. Starch modified with both Ac and OSA showed Tg even at low DSAc values, and glass transition temperature was increasing with increasing of DSAc. When the DSAc was higher than 1.06 the Tg dependence was not observed for dual modified samples.
| No | DSAc | DSOSA | Td, °C | Tg, °C | Contact angle, ° |
|---|---|---|---|---|---|
| 1 | 0 | 0 | 291 | - | 38 |
| 2 | 0.43 | 0 | 267 | - | 46 |
| 3 | 0.62 | 0 | 240 | - | 65 |
| 4 | 0.8 | 0 | 249 | 162 | 66 |
| 5 | 1.07 | 0 | 267 | 166 | 66 |
| 6 | 1.67 | 0 | 278 | 167 | 68 |
| 7 | 0 | 0.06 | 272 | - | 76 |
| 8 | 0.03 | 0.06 | 287 | 162 | 44 |
| 9 | 0.43 | 0.06 | 279 | 163 | 56 |
| 10 | 0.53 | 0.06 | 302 | 164 | 64 |
| 11 | 1.06 | 0.06 | 318 | 175 | 74 |
| 12 | 1.23 | 0.06 | 316 | 171 | 78 |
| 13 | 1.58 | 0.06 | 315 | 167 | 84 |
| 14 | 1.68 | 0.06 | 312 | 171 | 88 |
The hydrophobicity of starch acetate was gradually increasing with increasing DSAc (Table 1), as reflected by increasing water contact angle. Moreover, the modification of starch with octenyl succinic anhydride dramatically changed the hydrophobicity of starch i.e., the water contact angle of starch octenyl succinate with DS 0.06 was twice higher compared to that of native starch. Meanwhile, dual modified starch at low DSAc had lower contact angle than that of OSA starch. However, contact angle values increased with increment of DSAc reaching 88° for acetylated starch octenyl succinate with DSAc=1.68 and DSOSA=0.06.