Polyethylene terephthalate (PET) is one of the most used plastic in the world. It has properties such as high resistance of tensile and impact, high chemical resistance, transparency, easy machinability and high thermal stability [1, 2]. Due to these properties, PET is widely used in food and beverages packaging. Large consumption of PET is increasing the number of wastes in the world; therefore, nowadays there is very big problem of recycling.
There are known two PET recycling ways: mechanical and chemical [1]. During mechanical process, recycled PET (rPET) received, but quality of rPET is not as good as it could be [1]. Chemically recycling PET, there are known methods such as methanolysis, hydrolysis, aminolysis and glycolysis [1, 2]. The most popular method of PET recycling is glycolysis. Glycolysis recycling can be described as a depolymerization of PET polymer in ethylene glycol (EG) using different types of catalysts obtaining bis-2-hydroxyethylene terephthalate (BHET) monomer [1]. As the conditions and depolymerization process are not difficult, the other problem is the selection of metal catalysts to get the highest yield of BHET.
In this work, reaction was carried out in three-neck round bottom flask. Catalyst was added to EG solvent, heated until reflux (196 °C), then added PET and mixture was refluxed for 2.5 hours. Mayenite (Ca12Al14O33) was used as the catalyst for PET depolymerization. We used three types of mayenite with different calcination temperatures: 350, 550 and 900 °C. After 2.5 hours, the mixture was cooled in ice-bath, added boiling water and heated until 100 °C. To obtain BHET, the hot mixture was filtered. The filtrate was reheated until its clear, and then it was cooled to 5 °C and left for 16 h. The obtained crystals were dried at 60 °C. The reaction yield was calculated. The BHET structure was proved by FTIR analysis.
Tendencies were observed. The smaller amount of mayenite was added to reaction mixture the higher BHET yield was obtained, but mayenite concentration can not exceed 600 molls. The highest BHET yield was received using 600 molls of mayenite, which was calcinated in 900 °C. This mayenite has largest surface area and highest crystallinity.
| No. | Catalyst | mol/mol | g/g | Yield, % |
|---|---|---|---|---|
| 1 | 800 | 112.5 | 65.7 | |
| 2 | 600 | 84.4 | 69.2 | |
| 3 | Ca12Al14O33 (900 °C) | 400 | 56.2 | 64.4 |
| 4 | 200 | 28.2 | 50.6 | |
| 5 | 100 | 13.9 | 46.6 | |
| 6 | 800 | 108.7 | 48.2 | |
| 7 | 600 | 79.0 | 59.5 | |
| 8 | Ca12Al14O33 (550 °C) | 400 | 53.9 | 56.8 |
| 9 | 200 | 27.2 | 46.1 | |
| 10 | 100 | 14.0 | 22.4 | |
| 11 | 800 | 105.6 | 55.0 | |
| 12 | 600 | 83.4 | 55.8 | |
| 13 | Ca12Al14O33 (350 °C) | 400 | 54.7 | 56.1 |
| 14 | 200 | 28.4 | 45.3 | |
| 15 | 100 | 14.1 | 30.6 |